Causes and solutions for the brittleness of PVC plastic prof
欄目:Industry News 發布時間:2021-06-03 15:19
3. Too much or too little stabilizer The role of the stabilizer is to inhibit degradation or to react with the released hydrogen chloride and to prevent discoloration during processing of the polyvinyl chloride. Stabilizers vary by type, bu...


3. Too much or too little stabilizer
The role of the stabilizer is to inhibit degradation or to react with the released hydrogen chloride and to prevent discoloration during processing of the polyvinyl chloride.
Stabilizers vary by type, but in general, excessive use delays the plasticizing time of the material, resulting in less plasticization of the material as it exits the mold, and there is no complete fusion between them. The molecules in the formulation system.
Its intermolecular structure is not strong.
When the equivalent is too small, relatively low molecular substances in the formulation system may degrade or decompose (also referred to as excessive plasticization), and the stability of the intermolecular structure of each component may be destroyed.
Therefore, the amount of stabilizer also affects the impact strength of the profile. Too much or too little results in a reduction in profile strength and a tendency to make the profile brittle.
4, excessive use of external lubricants
The external lubricant is less soluble in the resin and promotes slippage between the resin particles, thereby reducing frictional heat and retarding the melting process. This effect of the lubricant is early in the process (ie, external heating and frictional heat generated internally).
The resin is the largest before the resin is completely melted, and the resin in the melt loses its identifying properties.
External lubricants are classified into pre-lubrication and post-lubrication, and over-lubricated materials exhibit poor shape under various conditions. If the lubricant is used improperly, it may cause flow marks, low yield, turbidity, poor impact, and rough surface.
, poor adhesion, poor plasticization, etc.
In particular, when the equivalent is too large, the compactness of the profile is poor, the plasticization property is poor, and the impact property is poor, resulting in the profile becoming brittle.
5, hot mixing feed sequence, temperature setting and curing time are also decisive factors for profile performance
There are many component formulas in PVC-U. The order of addition should be beneficial to the action of each additive, which is beneficial to increase the dispersion speed and avoid adverse synergistic effects. The order of the additives should help to improve the adjuvant.
The synergistic effect of the reagent overcomes the effect of phase elimination, so that the auxiliary agent which should be dispersed in the PVC resin completely enters the inside of the PVC resin.
The typical lead salt stabilization system recipe sequence is as follows:
a.
When running at low speed, add PVC resin to the hot mixing tank;
b.
Stabilizer and soap are added at 60 ° C under high speed operation;
c.
At 80 ° C, high speed operation, adding internal lubricants, pigments, impact modifiers, processing aids;
d.
Adding a lubricant such as wax at a high speed of about 100 ° C;
e.
Adding filler at high speed operation at 110 °C;
f.
The material is cooled in a cold mixing tank at a low speed of 110 ° C - 120 ° C;
g.
When the temperature of the mixture was cooled to about 40 ° C, the material was discharged and sieved.
The above feeding sequence is more reasonable, but in the actual production process, according to the equipment and various conditions, most manufacturers add other additives in addition to the resin.
There is also a light active calcium carbonate added together with a main component or the like.
This requires the company's technical staff to develop their own processing technology and feeding sequence according to the characteristics of the company.
In general, the hot mixing temperature is about 120 ° C, the temperature is too high
When the material is low, the gelation and the mixture are not uniform. Above this temperature, some substances may decompose and volatilize, and the dry mixed powder is yellow.
The mixing time is generally 7-10 minutes to achieve compaction, homogenization and partial gelation.
The cold mixture is usually below 40 ° C and the cooling time requirement is very short. If the temperature is above 40 ° C and the cooling rate is slow, the prepared dry mixture will be less dense than conventional.
The curing time of the dry mixture is usually 24 hours. When the time is longer than this, the material easily absorbs water or agglomerates. Below this time, the structure between the molecules is unstable, resulting in large fluctuations in the profile size and wall thickness during the extrusion process.
.
If the above link is not enhanced, the quality of the profile product will be affected. In some cases, the outline will be very fragile. (to be continued)
主站蜘蛛池模板: 亚洲欧美成人另类激情| 中文字幕一区二区人妻| 久久国产亚洲高清观看| 97se亚洲国产综合自在线| 国产欧美日韩在线中文一区| 狠狠色婷婷久久一区二区三区| 国产综合久久亚洲综合| 亚洲a片国产av一区无码| 在线观看无码不卡av| 亚洲精品无码mⅴ在线观看| 亚洲国产午夜精华无码福利| 一本久道久久综合狠狠老| 久久精品国产最新地址| 亚洲欧美色中文字幕在线| 国产精品久久久久久久伊一| 国产精品igao视频| 日韩人妻中文无码一区二区| 狠狠躁夜夜人人爽天96 | 人妻巨大乳一二三区| 国产99久久久国产精品~~牛| 精品无码一区二区三区不卡| 亚洲精品久久国产高清| 亚洲国产综合另类视频| 熟妇人妻中文字幕| 欧美野外疯狂做受xxxx高潮| 亚洲中文字幕精品久久久久久动漫| 亚洲中文字幕无码乱线久久视| 久久久久国产精品人妻aⅴ院| 久久大香香蕉国产拍国| 精品精品国产欧美在线| 国产色视频自在线观看| 久久精品国产精品亚洲38| 亚洲一线产区二线产区分布| 欧美日韩精品一区二区三区在线| av蓝导航精品导航| 精品国产一区二区三区久久久狼| 久久久久青草线蕉亚洲麻豆| 丰满少妇被猛烈进av毛片| 午夜大片男女免费观看爽爽爽尤物| 99日本精品永久免费久久| 国产色婷婷五月精品综合在线|