老司机午夜福利视频-国内精品久久人妻无码网站-韩国三级l中文字幕无码-久久精品国产久精国产思思-a欧美亚洲日韩在线观看

Ideas to analyze and solve the problem of rigid injection mo
欄目:Industry News 發(fā)布時(shí)間:2021-06-03 15:19
Basic reason: From the perspective of plastics, the occurrence of flash is due to the pressure in the mold cavity exceeding the clamping force, or due to damage to the mold. 1. First analyze the stage at which the flash is generated? (Fillin...
Basic reason: From the perspective of plastics, the occurrence of flash is due to the pressure in the mold cavity exceeding the clamping force, or due to damage to the mold.

1. First analyze the stage at which the flash is generated? (Filling stage, or filling stage)
1. First look at the filling process (short shot products) to determine whether to use a staged molding method;
2. Determine at which stage the flash occurs, whether it is the filling stage or the filling stage.

2. If the flash occurs during the filling stage
1. Reason analysis: Since the cavity is not filled during filling, it is usually not because the pressure in the cavity is too large to expand the mold beyond the clamping force, so the possible reasons are:
♦ During filling, the mold deforms;
♦ Damaged mold or poor coordination of fractal surface;
♦ Because the filling speed is too fast, or the plastic temperature is too high, the effective viscosity of the plastic is too low, and the flash appears in the area where the fractal surface is not tightly closed.
2. For different reasons, possible solutions are:
♦ Reduce the mold deformation by adding gaskets at the center of the template;
♦ Modify the mold;
♦ Slow down the injection speed or lower the plastic temperature.

3. If the flash occurs during the retraction phase
1. Reason analysis:
♦ The pressure in the cavity is too large, the clamping force is insufficient, and the mold is expanded;
♦ The filling speed is too slow, the effective viscosity of the plastic is too high, resulting in increased pressure loss in the cavity, and flash in areas where the pressure is too high;
♦ During packing, the mold deforms.
2. For different reasons, possible solutions are:
♦ Reduce the packing pressure or the packing rate, and check whether the clamping force is appropriate;
♦ Check the reason for the change of the effective viscosity of the plastic (the injection pressure integral during the filling phase), and adjust the process according to the specific reason;
♦ Measure the deformation of the mold to solve the mold deformation.
主站蜘蛛池模板: 亚洲精品久久一区二区三区四区 | 不卡无码人妻一区三区| 亚洲欧美成人久久一区| 色香阁综合无码国产在线| 亚洲偷自拍另类图片二区| 中国浓毛少妇毛茸茸| 妺妺窝人体色www在线| 性生交片免费无码看人| 亚洲人成线无码7777| 国产精品三级一区二区| 久久精品国产一区二区三| 国产精品99久久99久久久动漫| 国产成人喷潮在线观看 | 久久成人电影| 伊人精品成人久久综合97| 精品乱码一区内射人妻无码| 少妇又紧又色又爽又刺激视频| 女人高潮内射99精品| 国产99久久亚洲综合精品西瓜tv| 中国农村熟妇性视频| 欧美网站免费观看在线| 放荡的少妇2欧美版| 欧洲人妻丰满av无码久久不卡 | 国产成人精品一区二三区| 国产成人精品免费视频app软件 | 亚洲无av码一区二区三区| 2020年无码国产精品高清免费| 无码专区人妻诱中文字幕| 亚洲综合欧美在线一区在线播放| 国产成人国拍亚洲精品| 午夜熟女插插xx免费视频| 2019亚洲午夜无码天堂| 日韩高清亚洲日韩精品一区| 欧美高潮| 日韩在线 | 中文| 双乳被老汉揉搓a毛片免费观看| 亚洲人成色77777在线观看大战p| 一二三四区无产乱码1000集| 99国产成人综合久久精品77| 热99re6久精品国产首页| 亚洲欧美成αⅴ人在线观看|